POM (also known as SAI steel, Trim). It is obtained by polymerization of formaldehyde, etc. POM-H (polyacetal homopolymer), POM-K (polyacetal copolymer) is high-density, high crystallinity thermoplastic engineering plastics. They have good physical, mechanical, and chemical properties, especially excellent friction resistance.
POM is a crystalline plastic with an obvious melting point. Once the melting point is reached, the melt viscosity decreases rapidly. When the temperature exceeds a certain limit or the melt is heated for too long, it will cause decomposition. Copper is a POM degradation catalyst, and POM melt contact parts should avoid the use of copper or copper materials.
1. Plastic processingPOM water absorption is small, generally 0.2% -0.5%. Under normal circumstances, POM can be processed without drying, but the wet raw materials must be dried. Drying temperature above 80 ℃, time more than 2 hours, the specific should be carried out according to the supplier information.
The percentage of recycled material used is usually not more than 20-30%. However, depending on the type of product and end-use, sometimes up to 100%.
2. The choice of plastic machinePOM has no special requirements for
injection molding machines, except for the requirement of the screw without stagnant area, the general injection can be.
3. Mold and gate designCommon mold temperature control is 80-90℃, runner diameter is 3-6mm, the gate length is 0.5mm, gate size depends on the thickness of the rubber wall, round gate diameter should be at least 0.5-0.6 times the thickness of the product, rectangular gate width is usually 2 times or more than the thickness, depth is 0.6 times the wall thickness, demold slope is between 40′-130′.
Venting system.
POM-H thickness 0.01-0.02m, width 3mm
POM-K thickness 0.04mm, width 3mm
4. Melting speedMeasurable by air injection method.
POM-H can be set to 215℃ (190℃-230℃) POM-K can be set to 205℃ (190℃-210℃)
5. Injection speedIt is common for medium speed to be fast, too slow to produce ripples, too fast to produce shot lines, and shear overheating.
6. Back pressureThe lower the better, generally not more than 200bar.
7. Stagnation timeIf the equipment does not have a melt retention point POM-H can be retained at 215℃ for 35 minutes, POM-K can be retained at 205℃ for 20 minutes without serious decomposition, the melt cannot be retained in the barrel for more than 20 minutes at the injection temperature.
POM-K can be retained at 240°C for 7 minutes. If stop, the barrel temperature can be reduced to 150℃, if you want to stop for a long time, you must clean the barrel and turn off the heater.
8. ShutdownClean the barrel must use PE or PP, turn off the electric heater, and push the screw in the front position. The barrel and screw must be kept clean. Impurities or dirt will change the superheat stability of POM (especially POM-H). So when finished with halogen-containing polymers or other acidic polymers, apply PE to clean up before playing POM material, otherwise, an explosion will occur. If the role of improper pigments, lubricants, or materials containing GF nylon, will lead to plastic degradation.
9. Post-processingFor the very temperature use of the parts and high-quality requirements, the heat treatment shall be carried out.
Annealing treatment effect, you can put the product into the concentration of 30% hydrochloric acid solution for 30 minutes to check, and then use the naked eye to determine whether there are residual stress cracks.
Latest blog posts
Custom molds injection molding
Custom molds injection molding is a manufacturing process that involves creating custom molds to produce plastic parts. Injection molding is a popular technique used in various industries such as...
Plastic injection molding companies
Plastic injection molding is a manufacturing process that involves injecting molten plastic into a mold to create a wide range of plastic products. From car parts to medical devices and household items, plastic injection molding is used to create a variet
PET Preform Injection Moulding Machine
PET preform injection molding is a manufacturing process that is used to create PET (polyethylene terephthalate) preforms that can be later blown into bottles, jars, and other containers. This process...
You may like
Details that should be paid attention to before injection molding of fibrous PC
As we all know, the details determine success or failure, the best materials, even if you do not master a good detail, will be a loss. Especially fibrous PC plastic materials, in the injection molding modification process, must pay attention to the detail
What exactly is the relationship between mold size and plastic shrinkage?
When designing a plastic mold, after the mold structure is determined, the detailed design of each part of the mold can be carried out, i.e., the dimensions of each template...
Polishing treatment of plastic moulds
With the wide application of plastic products, such as daily chemical products and beverage packaging containers, the appearance needs often require the surface of plastic mold cavities to reach the degree of mirror polishing.
The premonition of injection molding machine failure and failure law before occurrence
The study of injection molding machine performance or condition gradually decreases with the time of use. Many failures are preceded by several precursors, which are called potential...